Silicon Carbide Ceramic Property

Corosion Test Results
Test Environment* Corrosive Weight Loss,mg/cm2/yr
Concentration Reagent, Wt% Temperature SiC SiSiC
98% H2SO4 100°C 1.5 50
50% NaOH 100°C 2.5 >1000
53% HF 100°C <0.2 7
85% H3PO4 100°C <0.2 8
70% HNO3 100°C <0.2 0.5
45% KOH 100°C <0.2 >1000
25% HCl 100°C <0.2 0.9
10% HF plus 57% HNO3 25°C <0.2 >1000
*125-300 hours of testing in all acids and continuously stirred.